GB 50661-2011 Code for welding of steel structures, Section 6.3: conditions requiring re-qualification of welding procedure for seven welding processes
GB 50661-2011 "Code for welding of steel structures" Section 6.3 (6.3.1-6.3.7), clause-by-clause by process, lists triggers for "re-qualification is required when any of the following conditions changes": shielded metal arc welding, GMAW/GTAW, submerged arc welding, electroslag welding, electrogas vertical welding, and stud welding each have explicit triggers — process parameters beyond the qualified allowable ranges (e.g., GMAW current/voltage/speed over 10%/7%/10%, stud welding key parameters over ±5%) require re-qualification.
Applicable Codes
- GB 50661-2011 · Code for Welding of Steel Structures Ch. 6 6.3节(6.3.1~6.3.7)
Topic Positioning
This card compiles all triggers of "re-qualification required when any of the following changes" for seven welding processes in Section 6.3 of Chapter 6 of GB 50661-2011 (mandatory national standard), for judging whether a qualified welding procedure still applies after changes in parameters, materials, or position.
Core Conclusions
[Shielded metal arc welding (6.3.1)] Re-qualify when any of: 1 tensile-strength class of electrode deposit changes; 2 low-hydrogen changed to non-low-hydrogen electrode; 3 electrode size changes; 4 current polarity of DC electrodes changes; 5 multi-pass changed to single-pass (or vice versa); 6 back-gouging changed to no back-gouging; 7 vertical-welding direction changes; 8 actual current/voltage outside the electrode datasheet's recommended range.
[GMAW — melting-electrode gas shielded (6.3.2)] 1 solid wire changed to flux-cored (or vice versa); 2 single shielding gas type changes; gas type or mix ratio of mixed gas changes; 3 gas flow increased >25% or decreased >10%; 4 torch weave width beyond ±20% of the qualified value; 5 actual current, voltage, and travel speed exceeding 10%, 7%, and 10% of qualified values respectively; 6 change between spray and short-circuit transfer; 7 wire classification changes; 8 wire diameter changes; 9 multi-pass/single-pass change; 10 back-gouging changed to no back-gouging.
[GTAW — non-melting-electrode gas shielded (6.3.3)] 1 shielding gas type changes; 2 gas flow increased >25% or decreased >10%; 3 adding filler or not; cold-wire vs hot-wire feed; filler type/strength class changes; 4 torch weave width beyond ±20% of the qualified value; 5 actual current and travel speed exceeding 25% and 50% of qualified values; 6 current polarity changes.
[Submerged arc welding (6.3.4)] 1 wire size changes; wire/flux classification changes; 2 multi-wire vs single-wire; 3 adding cold wire or not; 4 current type and polarity changes; 5 actual current, voltage, and speed exceeding 10%, 7%, and 15% of qualified values; 6 back-gouging changed to no back-gouging.
[Electroslag welding (6.3.5)] 1 single-wire vs multi-wire; plate electrode vs wire; with/without flux-consuming guide (melt tip); 2 guide cross-section changes >30%; guide brand changes; wire diameter changes; single/multi guide; flux classification changes; 3 single-sided vs double-sided groove; 4 current type and polarity changes; 5 power source characteristic changes constant-voltage vs constant-current; 6 actual current, voltage, wire-feed rate, and vertical travel exceeding 20%, 10%, 40%, and 20% of qualified values; 7 deviation from vertical >10 degrees; 8 change of water-cooled shoes/dams; 9 flux charge changes >30%.
[Electrogas vertical welding (6.3.6)] 1 wire classification and diameter; 2 shielding gas type or mix ratio; 3 gas flow increased >25% or decreased >10%; 4 current polarity; 5 actual current, wire-feed, and voltage exceeding 15%, 30%, and 10% of qualified values; 6 deviation from vertical >10 degrees; 7 change of water-cooled shoes/dams.
[Stud welding (6.3.7)] 1 stud material; 2 stud nominal diameter; 3 ferrule material; 4 non-through vs through-deck welding; 5 in through-deck welding, thickness of the pierced sheet, and coating weight/type; 6 position deviating >25 degrees from flat, or change among flat/horizontal/overhead; 7 stud welding method; 8 preheat 20 C lower or 50 C higher than qualified; 9 actual lift, stickout, time, current, and voltage varying beyond ±5% of qualified values; 10 with arc welding, welding consumable changes.
Background: the influence of parameters on joint quality differs by process; based on extensive tests, practice, and foreign standards, each clause fixes the maximum allowable variation of parameters per process.
Applicable Boundaries
- Section 6.3 addresses changes after qualification; any change beyond the above ranges voids the existing PQR and requires re-qualification.
- First-time adoption by the contractor (e.g., first domestic use of steel/consumables, or a first-time combination of materials, consumables, process, joint type, position, post-weld heat treatment, and parameters required by design) falls under initial qualification (Section 6.1), not "re-qualification".
- This card covers only Section 6.3 triggers; PQR preparation, test specimens, and validity periods (by welding difficulty grade, Clause 6.1.9) follow other clauses of Chapter 6.
Further Reading
- GB 50661-2011 Chapter 6 "Welding procedure qualification" Section 6.3 (6.3.1-6.3.7): SMAW, GMAW, GTAW, SAW, ESW, EGW, stud welding.
- Initial qualification conditions in Section 6.1; PQR validity and management in Clause 6.1.9.