Treatment requirements before continuing pours at construction joints/post-cast strips and the mortar bedding layer thickness limit (GB 50666-2011 cl. 8.3.10)

Per GB 50666-2011 cl. 8.3.10: before concreting at a construction joint or post-cast strip, the interface shall be roughened and cleared of laitance, loose stone and weak concrete; wetted by water but without standing water; the previously cast concrete at the joint shall have strength not less than 1.2MPa; the cement mortar bedding layer at horizontal joints of columns and walls shall not be thicker than 30mm and the mortar shall have the same composition as the concrete slurry; where the design is silent, post-cast strip concrete should be one grade stronger than both sides with shrinkage-reducing measures.

Applicable Codes

  • GB 50666-2011 · Code for Construction of Concrete Structures 第 8.3.10 条

Topic Positioning

Answers the workmanship-control questions "what treatment is required before continuing pours at construction joints/post-cast strips, and what is the thickness limit of the cement mortar bedding layer" in cast-in-place concrete construction, per GB 50666-2011 cl. 8.3.10 (Chapter 8, cast-in-place structural works) and its commentary.

Core Conclusions

GB 50666-2011 cl. 8.3.10 requires that concreting at construction joints or post-cast strips comply with the following:

  1. The interface shall be rough and cleared of laitance, loose stone and weak concrete layers. Where the joint or strip has been polluted by construction waste after long standing, the waste shall first be removed and the member repaired as necessary. The interface of staged pours of cast-in-place structures is also a type of construction joint.
  2. The interface shall be wetted with water but free of standing water. Thorough wetting ensures full bonding of new and old concrete; avoid ponded water which would impair bonding.
  3. The strength of the already cast concrete at the joint shall not be less than 1.2MPa. Below 1.2MPa the tight bonding of new and old concrete cannot be assured — this is the strength floor for continuing pours, not a design strength value.
  4. The bedding layer of cement mortar at horizontal construction joints of columns and walls shall not be thicker than 30mm, and the mortar shall have the same composition as the concrete slurry. Commentary: an over-thick bedding layer without coarse aggregate impairs the concrete strength grade; the maximum coarse aggregate is usually 25mm stone, so the layer is controlled below 30mm. 30mm is the upper limit; the clause sets no lower limit.
  5. The strength grade and properties of post-cast strip concrete shall satisfy the design; where the design is silent, the strength grade should be one grade higher than the concrete on both sides, with shrinkage-reducing technical measures. Commentary: post-cast strips are special locations in poor environments where bleeding may concentrate during pouring; raising one grade ensures quality; shrinkage-reducing measures include selection of constituents, mix design, placing methods and curing conditions.

Applicable Boundaries

Applies to workmanship control of continuing pours at construction joints and post-cast strips in building/municipal cast-in-place concrete works; the clause targets the "treatment before continuing pour" stage. 1.2MPa is the floor value of the cast concrete strength; 30mm is the upper limit of the bedding layer for horizontal joints of columns and walls — the commentary explains the value from the 25mm maximum coarse aggregate, and the thickness should be adjusted accordingly for other aggregate sizes. Other industry/local standards (hydraulic structures, city bridges, rail transit waterproofing etc.) may specify different bedding thicknesses or cast-concrete strengths; follow the standard actually applicable to the project, no mixing. This clause governs only joint/strip concreting; joint locations, formwork support and curing are elsewhere.

Further Reading

See GB 50666-2011 Chapter 8 "cast-in-place structural works", cl. 8.3.10 and commentary (direct source of the joint/strip concreting provisions); joint location requirements in cl. 8.3.9 of the same code; appearance quality and acceptance of concrete at joints and strips may be checked against the corresponding provisions of GB 50204-2015.

Keywords

  • 施工缝
  • 接浆层
  • 后浇带
  • 新老混凝土
  • GB 50666-2011
  • 混凝土结构工程施工规范
  • 1.2MPa
  • 粗糙面

Cited By